18禁无遮挡国产精品-欧美黄片在线视频免费观看-丰满人妻被粗大爽视频-亚洲永久精品中文字幕

產(chǎn)品展示
當(dāng)前位置:首頁 > 全部產(chǎn)品 > 英國Ossila > 材料 > Ossila材料PTB7 CAS:1266549-31-8 PTB7

Ossila材料PTB7 CAS:1266549-31-8 PTB7

Ossila材料PTB7 CAS:1266549-31-8 PTB7
Ossila代理、*、交期準(zhǔn)時(shí)、歡迎新老客戶?。?!

分享到:

只用于動物實(shí)驗(yàn)研究等

Batch Information

Batch No.MwPDStock Info
M21118,0001.75Sold out
M212> 40,0002.0Sold out
M21385,0002.0In stock

Ossila材料PTB7 CAS:1266549-31-8 PTB7

Applications

PTB7 for high-performance organic photovoltaics.

Poly[[4,8-bis[(2-ethylhexyl)oxy]benzo[1,2-b:4,5-b']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thieno[3,4-b]thiophenediyl]], more commonly known as PTB7.

In stock now for immediate dispatch worldwide.

PTB7 gives some of the highest reported efficiencies for polymer:fullerene solar cells due to its extended absorption into the near infra-red and lower HOMO level. Together with our complete package of processing information, PTB7 becomes a quick and easy way to improve device efficiencies. This represents a cost-effective method to increase performance and impact of devices and data for a wide range of OPV related research.

At typical concentrations for spin-coated devices of 10 mg/ml, a standard batch of 100 mg will produce 10 ml of ink - enough to coat 200 of Ossila's standard sized substrates even assuming 50% ink loss during preparation and filtration. At concentrations of 1 mg/ml (more typical for ink-jet printing and spray coating) up to 100 ml of ink can be produced.

In a standardised reference architecture (using a PEDOT:PSS hole interface and Ca/Al electron interface) we have shown this batch to give a PCE of 6.8% (see data sheet below) and up to 7.4% using PFN. By using new interface materials and architectures PTB7 has been shown to reach efficiencies of 9.2% PCE in the literature [1,2].

The high solubility in a wide range of solvents makes ink preparation and filtration simple, and PTB7 is one of the easiest materials we have ever worked with (simply shake it to dissolve). This also makes it an excellent candidate for a variety of coating techniques including ink-jet printing, spray coating and blade coating.

For information on processing please see our specific fabrication details for PTB7, general fabrication video, general fabrication guide, optical modelling paper on our standard architecture [3], or us for any additional help and support.

References (please note that Ossila has no formal connection to any of the authors or institutions in these references):

  • [1] Enhanced power-conversion efficiency in polymer solar cells using an inverted device structure Zhicai He et al., Nature Photonics, V 6, p591–595 (2012).
  • [2] Simultaneous Enhancement of Open-Circuit Voltage, Short-Circuit Current Density, and Fill Factor in Polymer Solar Cells Zhicai He et al., Advanced Materials, V 23, p4636–4643 (2011).
  • [3] Optimising the efficiency of carbazole co-polymer solar-cells by control over the metal cathode electrode Darren C. Watters et al., Organic Electronics, V 13, p1401–1408 (2012)
  • [4] Designing ternary blend bulk heterojunction solar cells with reduced carrier recombination and a fill factor of 77%, N. Gasparini et al, Nat. Energy, 16118 (2016); doi:10.1038/nenergy.2016.118 (Ossila PTB7 was featured in this paper).

Ossila材料PTB7 CAS:1266549-31-8 PTB7

Datasheet

PTB7 chemical structureChemical structure of PTB7; Chemical formula (C41H53FO4S4)n.

Specifications

Full namePoly[[4,8-bis[(2-ethylhexyl)oxy]benzo[1,2-b:4,5-b']dithiophene-2,6-diyl][3-fluoro-2-[(2-ethylhexyl)carbonyl]thieno[3,4-b]thiophenediyl]]
SynonymsPTB7
CAS number1266549-31-8
Absorption670 nm (CH2Cl2), 682 nm (film)
SolubilityChloroform, Chlorobenzene, o-DCB

 

Usage Details

Inverted Reference Devices

Reference device were made on batch M211 to assess the effect of PTB7:PC70BM active layer thickness on OPV efficiency using an inverted architecture with the below structure. These consisted of the below structure and were fabricated under inert atmosphere (glovebox) before encapsulation and measurement under ambient conditions.

Glass / ITO (100 nm) / PFN (6.5 nm) / PTB7:PC70BM (1:1.5) / MoOx (15 nm) / Al (100 nm)

For generic details please see the general fabrication guide and video. For specific details please see the below condensed fabrication report which details the optical modelling and optimisation of the multilayer stack.

Previously it has been shown that PFN of around 6.5 nm gives optimum performance [1-3,P021] while modelling has shown that an Al back cathode gives higher performance than Ag when used with MoOx [4].

The PTB7:PC70BM solution was made in chlorobenzene at 25 mg/ml before being diluted with 3% diiodooctane (DIO) to promote the correct morphology.

Active layer thicknesses of 75 nm, 90 nm and 105 nm were chosen corresponding to the lower, middle and upper end of the "thin film" absorption peak of a typical stack as predicted by optical modelling [1]. For each of these thickness a total of four substrates was produced, each with 4 pixels and the data presented below represents a non-subjective (no human intervention) analysis of the best 75% of pixels by PCE (12 pixels for each condition).

An additional two substrates were also prepared with a methanol wash to help remove the DIO as has been reported in the literature to help improve performance[5].

Overall, the maximum efficiency of 7.2% average PCE (7.4% maximum) was found at 75 nm film thickness.

 

Efficiency for different PTB7 spin speeds - inverted architectureJsc for different PTB7 spin speeds - inverted architectureVoc for different PTB7 spin speeds - inverted architecture Fill factor for different PTB7 spin speeds - inverted architectureFigure 1: PCE, Jsc, Voc and FF for inverted architecture devices at different spin speeds. Data shown is averaged with max and min overlaid with filled circles (please see note of Dektak measurements). As previously reported [1,2,3], films of approximay 90 nm give the highest performance with greater Jsc and only minor loss in fill factor.

 

PTB7 JV Curve for inverted architecture
Figure 2: The JV curve for the best performing device - inverted architecture.

 

Note 1: Dektak Thickness calibration

We normally calibrate thin films by use of a Dektak surface profiler, however the use of DIO results in an enhanced level of uncertainty in the film as the DIO will take several hours to fully dry under normal conditions and is likely to undergo some slight further shrinkage when placed in vacuum. The DIO can also be removed by baking the substrate on the hotplate at 80°C for about 10 mins which can be useful for doing quick measurements but also drives excess phase separation between the polymer and PCBM making it unsuitable for device work.

Note 2: Effect of epoxy

Due to the very high solubility of the PTB7 it was noted during fabrication that the film changed colour when in contact with the EE1 encapsulation epoxy in liquid form for extended periods indicating that there was some miscibility. Inspection of the active areas underneath the top cathode indicated that the epoxy had not seeped into the active area before curing and device metrics indicate that this did not appear to affect performance. However, we would recommend minimising contact time between the epoxy and PTB7 films before UV curing.

 

Fabrication

Substrates and cleaning

  • Pixelated Cathode substrates (S173)
  • 5 mins sonication in hot Hellmanex III(1 ml in beaker)
  • 2x boiling water dump rinses
  • 5 mins sonication in warm IPA
  • 2x dump rinses
  • 5 mins sonication in hot NaOH
  • Dump rinse in boiling water
  • Dump rinse in water
  • Stored in DI water overnight and until use

PFN Solution

  • Dissolved at 2 mg/ml
  • Acetic acid dissolved 1:9 in methanol to make stock solution
  • 2 μl/ml of acetic added to solution
  • Stirred for 30 mins
  • Filtered through 0.45 μm PVDF filter

PFN Test Films

  • PFN Test film initially spun at 500 rpm and gave 20 nm
  • Second test film spun at 1000 rpm and gave 16 nm
  • Thickness was extrapolated to 6.5 nm at 6000 rpm

Active Layer Solution

  • Fresh stock solutions of PTB7 (Ossila M211) made on at 10 mg/ml in CB and dissolved with stirbar for 1 hour
  • Mixed 1:1.5 with dry Ossila 99% C70 PCBM to make overall concentration of 25 mg/ml and dissolved with stirbar for 1 hour
  • Old stock solution of 1,8 Diiodooctane mixed 1:1 with CB to make measuring out small quantities easier
  • DIO/CB mixture added to solution to give overall DIO amount of 3%

Active Layer Test Films

  • Test film spun at 1000 rpm for 2 mins using unfiltered solution and dried using methanol before Dektak
  • 1000 rpm gave approximay 85 nm

Active layers

  • Devices spun using 30 μl dynamic dispense (20 μl gave only moderate wetting/coverage)
  • Non methanol devices spun for 2 mins
  • Methanol devices spun for 30 seconds, then coated with 50 μl methanol by static dispense then spun at 2000 rpm for 30 seconds.
  • Cathode wiped with CB
  • Vacuum dried in glovebox antichamber for 20 mins

Evaporation

Left in chamber over the weekend and evaporated with the below parameters.

  • 15 nm MoOx at 0.2 ?/s
  • 100 nm Al at 1.5 ?/s
  • Deposition pressure

Encapsulation

  • As standard using Ossila EE1, 30 mins UV in MEGA LV101

Measurements

  • JV sweeps taken with Keithley 237 source-meter
  • Illumination by Newport Oriel 9225-1000 solar simulator with 100 mW/cm2 AM1.5 output
  • NREL certified silicon reference cell used to calibrate
  • Lamp current: 7.8 A
  • Solar output at start of testing: 1.00 suns at 25°C
  • Solar output at end of testing: 1.00 suns at 25°C
  • Air cooled substrates
  • Room temperature at start of testing: 25°C
  • Room temperature at end of testing: 25°C
  • Calibrated aperture mask of size 0.256 mm2

 

Standard (Non-inverted) Reference Devices

Reference device were made on batch M211 using a standardised architecture for comparative measurements using Ossila standard substrates and materials. These consisted of the below structure and were fabricated under inert atmosphere (glovebox) before encapsulation and measurement under ambient conditions.

Glass / ITO (100 nm) / PEDOT:PSS (30 nm) / PTB7:PC70BM (variable) / Ca (2.5 nm) / Al (100 nm)

For generic details please see the fabrication guide and video. For specific details please see the below condensed fabrication report and also Watters et al. [3] which details the optical modelling and optimisation of the multilayer stack.

For this standard reference architecture an average PCE of 6.6% was achieved for the optimised thickness with a peak efficiency of 6.8%. Note that no other optimisation was performed (blend ratio, DIO concentration, drying conditions etc) and so further small improvements may be obtained by varying these conditions and significant improvements obtained by using alternative interface materials [1,2].

Efficiency for different PTB7 spin speeds - Standard architecture Jsc for different PTB7 spin speeds - Standard architecture Voc for different PTB7 spin speeds - Standard architecture Fill factor for different PTB7 spin speeds - Standard architectureFigure 3: PCE, Jsc, Voc and FF for standard architecture devices at different spin speeds. Data shown is averaged with max and min overlaid with filled circles (please see note of Dektak measurements). As previously reported [1,2,3], films of approximay 90 nm give the highest performance with greater Jsc and only minor loss in fill factor.

 

PTB7 JV curve for standard architecture
Figure 4: The JV curve for the best performing device - standard architecture.

 

Note 1: Dektak Thickness calibration

We normally calibrate thin films by use of a Dektak surface profiler, however the use of DIO results in an enhanced level of uncertainty in the film as the DIO will take several hours to fully dry under normal conditions and is likely to undergo some slight further shrinkage when placed in vacuum. The DIO can also be removed by baking the substrate on the hotplate at 80°C for about 10 mins which can be useful for doing quick measurements but also drives excess phase separation between the polymer and PCBM making it unsuitable for device work.

Note 2: Effect of epoxy

Due to the very high solubility of the PTB7 it was noted during fabrication that the film changed colour when in contact with the EE1 encapsulation epoxy in liquid form for extended periods indicating that there was some miscibility. Inspection of the active areas underneath the top cathode indicated that the epoxy had not seeped into the active area before curing and device metrics indicate that this did not appear to affect performance. However, we would recommend minimising contact time between the epoxy and PTB7 films before UV curing.

 

Fabrication

Substrates and cleaning

  • Pixelated Cathode substrates (S173)
  • 5 mins sonication in hot Hellmanex (1 ml in beaker)
  • 2x boiling water dump rinses
  • 5 mins sonication in warm IPA
  • 2x dump rinses
  • 5 mins sonication in hot NaOH
  • Dump rinse in boiling water
  • Dump rinse in water
  • Stored in DI water overnight and until use

PEDOT:PSS layer preparation

  • Clevios AI 4083
  • Filtered into vial using Whatman 0.45 μm PVDF filter
  • Spun 6000 rpm for 30 seconds (30 nm)
  • Dynamic dispense of 20 μl using pipettor
  • IPA cathode strip wipe and labelled
  • Put straight onto hotplate at 160°C as soon as cathode wiped and labelled
  • Transferred to glovebox when all samples spun.
  • Baked in glovebox at 150°C for 1 hour

Active layer Solution Preparation

  • Fresh stock solutions of PTB7 at 10 mg/ml in CB and shaken to dissolve
  • Mixed 1:1.5 with dry Ossila 99% C70 PCBM to make overall concentration of 25 mg/ml
  • 1,8 Diiodooctane mixed 1:1 with CB to make measuring out small quantities easier
  • DIO/CB mixture added to solution to give overall DIO amount of 3%

Active layer spin casting

  • Devices spun for 2 mins using 25 μl dynamic dispense
  • Cathode wiped with chlorobenzene
  • Left to dry in glovebox for 2 hours but colour indicated they were still slightly wet
  • Dried in vacuum in glovebox antichamber for 10 mins to remove DIO

Evaporation

Left in chamber over the weekend and evaporated with the below parameters.

MaterialCa
Base pressure8.0 E-8 mbar
Dep start pressure1.7 E-7 mbar
Max pressure2.7 E-7 mbar
Thickness2.5 nm
Rate0.2 ?/s
MaterialAl
Base pressure7.0 E-8 mbar
Dep start pressure6.0 E-7 mbar
Max pressure7.0 E-7 mbar
Thickness100 nm
Rate1.0 ?/s

 Encapsulation

  • As standard using Ossila EE1, 30 mins UV in MEGA LV101

Measurements

  • JV sweeps taken with Keithley 237 source-meter
  • Illumination by Newport Oriel 9225-1000 solar simulator with 100 mW/cm2 AM1.5 output
  • NREL certified silicon reference cell used to calibrate
  • Lamp current: 7.8 A
  • Solar output at start of testing: 0.99 suns at 25°C
  • Solar output at end of testing: 1.00 suns at 25°C
  • Air cooled substrates
  • Room temperature at start of testing: 21°C
  • Room temperature at end of testing: 21°C
  • Calibrated aperture mask of size 0.256 mm2

 

留言框

  • 產(chǎn)品:

  • 您的單位:

  • 您的姓名:

  • 聯(lián)系電話:

  • 常用郵箱:

  • 省份:

  • 詳細(xì)地址:

  • 補(bǔ)充說明:

  • 驗(yàn)證碼:

    請輸入計(jì)算結(jié)果(填寫阿拉伯?dāng)?shù)字),如:三加四=7

深圳市澤拓生物科技有限公司是國內(nèi)專業(yè)的Ossila材料PTB7 CAS:1266549-31-8 PTB7廠家,歡迎廣大顧客來電咨詢!
深圳市澤拓生物科技有限公司版權(quán)所有   |   技術(shù)支持:化工儀器網(wǎng)
聯(lián)系電話:0755-23003036   傳真:0755-23003036-807 GoogleSitemap 備案號:粵ICP備17105262號  管理登陸
在線客服
用心服務(wù)成就你我
国产视频一区一区二区| 日韩精品中文女同在线播放| 日本岛国一区二区在线| 熟伦熟女高潮露脸专区| av在线视频男人的天堂| 国产真实精品对白又爽欧美| 日韩精品视频网址进入| av网址一区二区三区| 欧美日韩亚洲激情一区| 男人一区二区在线观看| 宅男在线视频免费播放| 国产精品乱码一区二区视频| 欧美女人又粗又长亚洲| 成人一区二区三区蜜桃| 91成人国产在线视频| 午夜高清影院免费观看| 91精品国产免费人成网站| 一区二区三区亚洲天堂| 久草尤物视频在线观看| 伦理视频一区二区三区在线观看| 国产视频高清在线不卡| 日本中文字幕区二区三区电影| 国产精品国产三级国产专播下| 亚洲综合在不卡在线另类国产| 国产美女视频一区二区三区白浆 | 国产九九视频一区二区三区| 亚洲av二区三区在线| 亚洲成人爱情动作片在线播放| 久久婷婷av一区二区三区| 国产一区二区三区免费在线 | 夫妻在线观看高清视频 | av一区二区三区网站| 亚洲男人的天堂一区二区| 日韩av一区二区三区播放| 每日更新中文字幕粉嫩av| 亚洲av午夜福利久久精品| 久久国产高清亚洲电影| 色欧美一区二区三区在线| 一级精品水蜜桃少妇免费观看| 九色精品国产亚洲av麻豆一| 国产少妇露脸精品自拍网站|